True Stress - True Strain Curve: Part Four

Sommario:

This article describes strain-hardening exponent and strength coefficient, materials constants which are used in calculations for stress-strain behaviour in work hardening, and their application in some of the most commonly used formulas, such as Ludwig equation.

The flow curve of many metals in the region of uniform plastic deformation can be expressed by the simple power curve relation

(10)

where n is the strain-hardening exponent and K is the strength coefficient. A log-log plot of true stress and true strain up to maximum load will result in a straight-line if Eq. (10) is satisfied by the data (Fig. 1).

The linear slope of this line is n and K is the true stress at e = 1.0 (corresponds to q = 0.63). The strain-hardening exponent may have values from n = 0 (perfectly plastic solid) to n = 1 (elastic solid), see Fig. 2. For most metals n has values between 0.10 and 0.50, see Table 1.

It is important to note that the rate of strain hardening ds /de, is not identical with the strain-hardening exponent. From the definition of n

or

(11)

Figure 2. Log/log plot of true stress-strain curve


Figure 3. Various forms of power curve s=K* e n


Table 1. Values for n and K for metals at room temperature

Metal Condition n K, psi
0,05% C steel Annealed 0,26 77000
SAE 4340 steel Annealed 0,15 93000
0,60% C steel Quenched and tempered 1000oF 0,10 228000
0,60% C steel Quenched and tempered 1300oF 0,19 178000
Copper Annealed 0,54 46400
70/30 brass Annealed 0,49 130000


There is nothing basic about Eq. (10) and deviations from this relationship frequently are observed, often at low strains (10-3) or high strains (1,0).

One common type of deviation is for a log-log plot of Eq. (10) to result in two straight lines with different slopes. Sometimes data which do not plot according to Eq. (10) will yield a straight line according to the relationship

(12)

Datsko has shown how e0, can be considered to be the amount of strain hardening that the material received prior to the tension test.

Another common variation on Eq. (10) is the Ludwig equation

(13)

where s0 is the yield stress and K and n are the same constants as in Eq. (10). This equation may be more satisfying than Eq. (10) since the latter implies that at zero true strain the stress is zero.

Morrison has shown that s0 can be obtained from the intercept of the strain-hardening point of the stress-strain curve and the elastic modulus line by


The true-stress-true-strain curve of metals such as austenitic stainless steel, which deviate markedly from Eq. (10) at low strains, can be expressed by


where eK is approximately equal to the proportional limit and n1 is the slope of the deviation of stress from Eq. (10) plotted against e. Still other expressions for the flow curve have been discussed in the literature.

The true strain term in Eqs.(10) to (13) properly should be the plastic strain

ep= etotal- eE= etotal- s/E

Criteri di ricerca
Inserite il vostro testo in inglese per la ricerca:

Ricerca tramite

Ricerca tramite

Testo completo
Intestazioni

Articolo
Sommario

Questo Articolo fa parte di una serie di Articoli di tecnologia metallurgica. È possibile fare clic sui link qui sotto per saperne di più su questo argomento.

Il Modulo opzionale Extended Range di Total Materia include una raccolta unica al mondo di curve Stress-Strain per calcoli in campo plastico relativi a migliaia di leghe metalliche, per differenti Trattamenti Termici e temperature di lavoro. Curve "true" e "engineering" sono fornite per varie velocità di deformazione ove applicabili.

Trovare un grafico Stress-Strain nel database è semplice e richiede solo pochi secondi.

Per prima cosa occorre inserire la Designazione della lega che interessa nel campo di Ricerca Rapida. Opzionalmente si può restringere la ricerca selezionando il Paese / Normativa dalla lista a discesa, e poi si clicca su "Invio".


Dopo aver selezionato il materiale di interesse, occorre cliccare sul collegamento "Curve Stress-Strain" per visualizzare i dati relativi al materiale selezionato. Il numero dei dati (diagrammi) disponibili viene visualizzato tra parentesi accanto al link.


Perché le curve Stress-Strain sono neutrali rispetto alle Normative, è possibile visualizzare i diagrammi cliccando sul link relativo per ogni Sottogruppo.

Oltre le curve Stress-Strain a diverse temperature, i dati sono forniti in forma di tabella che è esportabile a un software CAE come testo.


È anche possibile visualizzare curve Stress-Strain e relativi dati numerici per diverse temperature di lavoro.

Per fare questo, è sufficiente inserire una nuova temperatura nella casella specifica compresa nei limiti definiti e dare Invio.

Dopo aver fatto clic sul pulsante "Calcola", viene generata una nuova curva e i valori nella tabella corrispondono ora alla nuova temperatura. Si veda l'esempio qui sotto per 250°C.


Per consentirvi di testare il Database Total Materia "senza impegno", vi invitiamo a unirvi alla comunità degli Utenti registrati per i test gratuiti a Total Materia.