1.3342 (European Union / EN) Material Properties

Other designations:
Material group: Ferrous Alloys / Tool steels
Country/Standard: European Union / EN

Data updates

Latest Update: 2023-10
Total number of updates: 3
Update History:
2022-09 2018-09

Mechanical Properties


Temperature

0 - 30°C
PROPERTY / VALUE
Brinell Hardness (HB) ≤ 269 view details
Rockwell Hardness (HR) 48 view details
Brinell Hardness (HB) ≤ 269 view details
Rockwell Hardness (HR) 48 view details

Physical Properties


Temperature

0 - 30°C
30 - 100°C
100 - 300°C
≥ 300°C
PROPERTY / VALUE
Modulus of Elasticity 190 — 217 GPa view details
Shear Modulus val1
Full data access requires a free trial. Sign Up Free
GPa
view details
Density val1
Full data access requires a free trial. Sign Up Free
kg/dm³
view details
Poisson Coefficient val1
Full data access requires a free trial. Sign Up Free
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Thermal Conductivity 19 W/(m∙°C) view details
Heat Capacity val1
Full data access requires a free trial. Sign Up Free
J/(kg∙°C)
view details
Electrical Resistivity 0.54 Ω∙mm²/m view details
Electrical Conductivity val1
Full data access requires a free trial. Sign Up Free
S/m
view details
Modulus of Elasticity 27.6 E+03 — 31.5 E+03 ksi view details
Shear Modulus val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Density val1
Full data access requires a free trial. Sign Up Free
lb/in³
view details
Poisson Coefficient val1
Full data access requires a free trial. Sign Up Free
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Thermal Conductivity 11 BTU/(h∙ft∙°F) view details
Heat Capacity val1
Full data access requires a free trial. Sign Up Free
BTU/(lb∙°F)
view details
Electrical Resistivity 898 E-06 Ω∙circular·mil/ft view details
Electrical Conductivity val1
Full data access requires a free trial. Sign Up Free
S/in
view details

Composition

CRITERIA
VALUE
UNIT
CAS NUMBER
CRITERIA
C
VALUE
0.86 – 0.94
UNIT
%
CAS NUMBER
7440-44-0
CRITERIA
Cr
VALUE
3.8 – 4.5
UNIT
%
CAS NUMBER
7440-47-3
CRITERIA
Mn
VALUE
≤ 0.40
UNIT
%
CAS NUMBER
7439-96-5
CRITERIA
Mo
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7439-98-7
CRITERIA
P
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7723-14-0
CRITERIA
S
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7704-34-9
CRITERIA
Si
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-21-3
CRITERIA
V
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-62-2
CRITERIA
W
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-33-7

EN ISO 4957: 2018 / Tool steels

Heat Treatments

  • Austenitized at 1210 ± 10°C and quenched. Usual quenching media in practice are air, gas or salt bath. Total heating time of test pieces in a salt bath is 3 min. for hardening and minimum 2 periods of 60 min. each for tempering.<br />Tempered at 560 ± 10°C.