Mechanical Properties


Temperature

0 - 30°C
PROPERTY / VALUE
Tensile Strength 75 MPa view details
Elongation, A 10 % view details
Brinell Hardness (HB) 17 view details
Tensile Strength 10.9 ksi view details
Elongation, A 10 % view details
Brinell Hardness (HB) 17 view details

Physical Properties


Temperature

0 - 30°C
30 - 100°C
100 - 300°C
PROPERTY / VALUE
Modulus of Elasticity 69 — 79 GPa view details
Density val1
Full data access requires a free trial. Sign Up Free
kg/dm³
view details
Poisson Coefficient val1
Full data access requires a free trial. Sign Up Free
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Thermal Conductivity 180 — 210 W/(m∙°C) view details
Electrical Resistivity 0.029 Ω∙mm²/m view details
Electrical Conductivity val1
Full data access requires a free trial. Sign Up Free
S/m
view details
Modulus of Elasticity 10 E+03 — 11.5 E+03 ksi view details
Density val1
Full data access requires a free trial. Sign Up Free
lb/in³
view details
Poisson Coefficient val1
Full data access requires a free trial. Sign Up Free
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Thermal Conductivity 104 — 121 BTU/(h∙ft∙°F) view details
Electrical Resistivity 48.9 E-06 Ω∙circular·mil/ft view details
Electrical Conductivity val1
Full data access requires a free trial. Sign Up Free
S/in
view details

Composition

CRITERIA
VALUE
UNIT
CAS NUMBER
CRITERIA
Al
VALUE
≥ 99.7000
UNIT
%
CAS NUMBER
7429-90-5
CRITERIA
B
VALUE
≤ 0.04
UNIT
%
CAS NUMBER
7440-42-8
CRITERIA
Cr
VALUE
≤ 0.004
UNIT
%
CAS NUMBER
7440-47-3
CRITERIA
Cr+Mn+Ti+V
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
CRITERIA
Cu
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-50-8
CRITERIA
Fe
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7439-89-6
CRITERIA
Mn
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7439-96-5
CRITERIA
Other each
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
CRITERIA
Si
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-21-3

EN 576: 2003 / Aluminium and aluminium alloys - Unalloyed aluminium ingots for remelting - Specifications

Heat Treatments

Since direct data is not available in the original source, register for a free trial to explore similar or equivalent materials having these properties.

Register Now