EN-GJLA-XNiMn13-7 (European Union / EN) Material Properties

Other designations: ,
Material group: Ferrous Alloys / Cast irons
Country/Standard: European Union / EN

Data updates

Latest Update: 2022-10
Total number of updates: 5
Update History:
2016-10 2015-12 2015-09 2015-02

Mechanical Properties


Temperature

0 - 30°C
PROPERTY / VALUE
Tensile Strength 90 — 220 MPa view details
Compression Strength 630 — 840 MPa view details
Brinell Hardness (HB) 120 — 150 view details
Tensile Strength 13.1 — 31.9 ksi view details
Compression Strength 91.37 — 121.83 ksi view details
Brinell Hardness (HB) 120 — 150 view details

Physical Properties


Temperature

0 - 30°C
30 - 100°C
100 - 300°C
≥ 300°C
PROPERTY / VALUE
Modulus of Elasticity 70 — 90 GPa view details
Modulus of Elasticity val1
Full data access requires a free trial. Sign Up Free
GPa
view details
Modulus of Elasticity val1
Full data access requires a free trial. Sign Up Free
GPa
view details
Modulus of Elasticity val1
Full data access requires a free trial. Sign Up Free
GPa
view details
Density val1
Full data access requires a free trial. Sign Up Free
kg/dm³
view details
Poisson Coefficient val1
Full data access requires a free trial. Sign Up Free
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Thermal Conductivity 39 W/(m∙°C) view details
Heat Capacity val1
Full data access requires a free trial. Sign Up Free
J/(kg∙°C)
view details
Electrical Resistivity 1.2 Ω∙mm²/m view details
Electrical Conductivity val1
Full data access requires a free trial. Sign Up Free
S/m
view details
Modulus of Elasticity 10.2 E+03 — 13.1 E+03 ksi view details
Modulus of Elasticity val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Modulus of Elasticity val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Modulus of Elasticity val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Density val1
Full data access requires a free trial. Sign Up Free
lb/in³
view details
Poisson Coefficient val1
Full data access requires a free trial. Sign Up Free
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Thermal Conductivity 22.5 BTU/(h∙ft∙°F) view details
Heat Capacity val1
Full data access requires a free trial. Sign Up Free
BTU/(lb∙°F)
view details
Electrical Resistivity 1.99 E-03 Ω∙circular·mil/ft view details
Electrical Conductivity val1
Full data access requires a free trial. Sign Up Free
S/in
view details

Composition

CRITERIA
VALUE
UNIT
CAS NUMBER
CRITERIA
C
VALUE
≤ 3.0000
UNIT
%
CAS NUMBER
7440-44-0
CRITERIA
Cr
VALUE
≤ 0.2000
UNIT
%
CAS NUMBER
7440-47-3
CRITERIA
Cu
VALUE
≤ 0.5
UNIT
%
CAS NUMBER
7440-50-8
CRITERIA
Mn
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7439-96-5
CRITERIA
Ni
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-02-0
CRITERIA
P
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7723-14-0
CRITERIA
Si
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-21-3

EN 13835: 2012 / Founding - Austenitic cast irons

Heat Treatments

  • Stress relieving: heat up to between 625-650°C at a rate not exceeding 150°C/h, hold within this range for 2 h plus 1 h per 25 mm section thickness, cool down to 200°C in the furnace at a rate not exceeding 100°C/h, air cool. Heat treatment for high temperature stability: heat up to between 875-900°C at a rate not exceeding 150°C/h, hold within this range for 2 h plus 1 h per 25 mm section thickness, cool down to 500°C in the furnace at a rate not exceeding 50°C/h, air cool.