Mechanical Properties


Temperature

0 - 30°C
30 - 100°C
100 - 300°C
≥ 300°C
PROPERTY / VALUE
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
MPa
view details
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
MPa
view details
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
MPa
view details
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
MPa
view details
Tensile Strength 590 — 790 MPa view details
Elongation, A 12 % view details
Impact Energy val1
Full data access requires a free trial. Sign Up Free
J
view details
Brinell Hardness (HB) 170 — 240 view details
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Tensile Strength 85.6 — 114.6 ksi view details
Elongation, A 12 % view details
Impact Energy val1
Full data access requires a free trial. Sign Up Free
ft·lb
view details
Brinell Hardness (HB) 170 — 240 view details

Physical Properties


Temperature

0 - 30°C
30 - 100°C
100 - 300°C
≥ 300°C
PROPERTY / VALUE
Density 7.7 kg/dm³ view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Thermal Conductivity 29 W/(m∙°C) view details
Heat Capacity 460 J/(kg∙°C) view details
Density 0.278 lb/in³ view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Thermal Conductivity 16.8 BTU/(h∙ft∙°F) view details
Heat Capacity 0.11 BTU/(lb∙°F) view details

Composition

CRITERIA
VALUE
UNIT
CAS NUMBER
CRITERIA
C
VALUE
0.16 – 0.23
UNIT
%
CAS NUMBER
7440-44-0
CRITERIA
Cr
VALUE
12.50 – 14.50
UNIT
%
CAS NUMBER
7440-47-3
CRITERIA
Cu
VALUE
≤ 0.30
UNIT
%
CAS NUMBER
7440-50-8
CRITERIA
Mn
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7439-96-5
CRITERIA
Ni
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-02-0
CRITERIA
P
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7723-14-0
CRITERIA
S
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7704-34-9
CRITERIA
Si
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-21-3
CRITERIA
V
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-62-2

EN 10283: 2019 / Corrosion resistant steel castings

Heat Treatments

  • <b> Quenching (+Q) </b> at 950 to 1050°C in air or liquid. <br> <b>Tempering (+T) </b> at 650 to 750°C.
  • Annealing at 750 - 800°C, furnace cooling. Quenching at 1000 - 1050°C, air quenching. Tempering at 650 - 750°C.