1.1192 (Germany / DIN) Material Properties

Other designations: , ,
Material group: Ferrous Alloys / Structural and constructional steels
Country/Standard: Germany / DIN

Data updates

Latest Update: 2021-05
Total number of updates: 4
Update History:
2020-08 2018-01 2015-07

Mechanical Properties


Temperature

0 - 30°C
PROPERTY / VALUE
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
MPa
view details
Tensile Strength 570 MPa view details
Elongation, A 14 % view details
Reduction of Area val1
Full data access requires a free trial. Sign Up Free
%
view details
Shear Strength 460 MPa view details
Impact Energy val1
Full data access requires a free trial. Sign Up Free
J
view details
Rockwell Hardness (HR) val1
Full data access requires a free trial. Sign Up Free
view details
Yield Strength, Rp0.2 val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Tensile Strength 82.7 ksi view details
Elongation, A 14 % view details
Reduction of Area val1
Full data access requires a free trial. Sign Up Free
%
view details
Shear Strength 66.7 ksi view details
Impact Energy val1
Full data access requires a free trial. Sign Up Free
ft·lb
view details
Rockwell Hardness (HR) val1
Full data access requires a free trial. Sign Up Free
view details

Physical Properties


Temperature

0 - 30°C
30 - 100°C
100 - 300°C
PROPERTY / VALUE
Modulus of Elasticity 190 — 210 GPa view details
Density 7.67 — 7.86 kg/dm³ view details
Poisson Coefficient 0.27 — 0.3 view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Modulus of Elasticity 27.6 E+03 — 30.5 E+03 ksi view details
Density 0.277 — 0.284 lb/in³ view details
Poisson Coefficient 0.27 — 0.3 view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details

Composition

CRITERIA
VALUE
UNIT
CAS NUMBER
CRITERIA
C
VALUE
0.4200 – 0.5000
UNIT
%
CAS NUMBER
7440-44-0
CRITERIA
Mn
VALUE
0.5000 – 0.8000
UNIT
%
CAS NUMBER
7439-96-5
CRITERIA
P
VALUE
≤ 0.0350
UNIT
%
CAS NUMBER
7723-14-0
CRITERIA
S
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7704-34-9
CRITERIA
Si
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-21-3

DIN 1654-4: 1989 / Cold heading and cold extruding steels; technical delivery conditions for steels for quenching and tempering

Heat Treatments

  • Austenizing temperature: 850 ± 5°C
  • Hardening (quenching in water or oil): 820-860°C; Tempering: 540-680°C; Normalizing: 840-870°C