Mechanical Properties


Temperature

0 - 30°C
PROPERTY / VALUE
Tensile Strength 800 MPa view details
Brinell Hardness (HB) 156 — 270 view details
Grain Size Fine grain steel shall have an austenite grain size of 5 or finer. Sampling and sample preparation shall be as specified in ISO 643. The grain size shall be determined from a carburized specimen. Carburization shall be achieved by maintaining the specimen in carburizing powder at 950°C ± 10°C for 6 h. This is generally done by keeping the carburizing chamber at 950°C ± 10°C for 8 h, including a preheating period. In most cases, a carburized layer of approximately 1 mm is obtained.; Steel shall have an austenite grain size of 5 or finer in accordance with ISO 643. view details
Tensile Strength 116 ksi view details
Brinell Hardness (HB) 156 — 270 view details
Grain Size Fine grain steel shall have an austenite grain size of 5 or finer. Sampling and sample preparation shall be as specified in ISO 643. The grain size shall be determined from a carburized specimen. Carburization shall be achieved by maintaining the specimen in carburizing powder at 950°C ± 10°C for 6 h. This is generally done by keeping the carburizing chamber at 950°C ± 10°C for 8 h, including a preheating period. In most cases, a carburized layer of approximately 1 mm is obtained.; Steel shall have an austenite grain size of 5 or finer in accordance with ISO 643. view details

Physical Properties


Temperature

0 - 30°C
30 - 100°C
100 - 300°C
≥ 300°C
PROPERTY / VALUE
Modulus of Elasticity 190 — 210 GPa view details
Shear Modulus val1
Full data access requires a free trial. Sign Up Free
GPa
view details
Density val1
Full data access requires a free trial. Sign Up Free
kg/dm³
view details
Poisson Coefficient val1
Full data access requires a free trial. Sign Up Free
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°C
view details
Thermal Conductivity 38 W/(m∙°C) view details
Heat Capacity val1
Full data access requires a free trial. Sign Up Free
J/(kg∙°C)
view details
Electrical Resistivity 0.18 Ω∙mm²/m view details
Modulus of Elasticity 27.6 E+03 — 30.5 E+03 ksi view details
Shear Modulus val1
Full data access requires a free trial. Sign Up Free
ksi
view details
Density val1
Full data access requires a free trial. Sign Up Free
lb/in³
view details
Poisson Coefficient val1
Full data access requires a free trial. Sign Up Free
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Coefficient of Thermal Expansion (CTE) val1
Full data access requires a free trial. Sign Up Free
10-6/°F
view details
Thermal Conductivity 22 BTU/(h∙ft∙°F) view details
Heat Capacity val1
Full data access requires a free trial. Sign Up Free
BTU/(lb∙°F)
view details
Electrical Resistivity 299 E-06 Ω∙circular·mil/ft view details

Composition

CRITERIA
VALUE
UNIT
CAS NUMBER
CRITERIA
C
VALUE
0.13 – 0.19
UNIT
%
CAS NUMBER
7440-44-0
CRITERIA
Cr
VALUE
0.60 – 1.00
UNIT
%
CAS NUMBER
7440-47-3
CRITERIA
Mn
VALUE
0.70 – 1.00
UNIT
%
CAS NUMBER
7439-96-5
CRITERIA
Ni
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-02-0
CRITERIA
P
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7723-14-0
CRITERIA
S
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7704-34-9
CRITERIA
Si
VALUE
val1
Full data access requires a free trial. Sign Up Free
UNIT
%
CAS NUMBER
7440-21-3

EN 10084: 2008 / Case hardening steels - Technical delivery conditions

Heat Treatments

  • End quench test: Quench from 880°C Carburizing: 880 to 980°C; NOTE: If steels are direct hardened, in general, a carburizing temperature of 950°C is not exceeded. For special procedures, for example under vacuum, higher temperatures (for example 1020 to 1050°C) are not unusual. Core hardening: 850 to 890°C; Case hardening: 780 to 820°C; Tempering: 150 to 200°C (as a guide, for 1 hour minimum).
  • End quench test austenitizing at 880 ± 5°C (Time for austenitizing as a guide: 30 min minimum);<br><br>Carburizing at 880-980°C (The carburizing temperature depends on the chemical composition of the steel, the mass of the product and the carburizing medium. If the steels are direct hardened, in general, a temperature of 950°C is not exceeded. For special procedures, for example under vacuum, higher temperatures (for example 1020-1050°C) are not unusual);<br><br>Direct and simple hardening at 820-860°C (The kind of quenching agent depends on, for example the shape of the products, the cooling conditions and the amount of furnace filling. If the steels are direct hardened and if there is a danger of distortion, they should be quenched from a temperature between the core-hardening and case-hardening temperatures);<br><br>Double hardening: Core-hardening at 850-890°C and Case-hardening at 780-820°C;<br><br>Tempering at 150-200°C (Time for tempering as a guide: 1h minimum).